Value chains › Building Materials
Building materials (concrete blocks and pavers)
Dry mixes by % weight of cement, quarry dust and 6 mm ballast; blocks and pavers pressed on moulds counted in cycles; fresh stock goes to the curing yard (quarantine) and is released only after the curing days and a compressive-strength test; sold by the piece, the pallet or the m².
mfg.building_materials
Formulation and mixing example yields, to be confirmed at the factory
What the factory receives
Raw material your system can send as a consignment (item.code):
| Item | Code | Unit | HS code |
|---|---|---|---|
| Cement CEM II 32.5N | CEMENT-32.5 | kg | 2523.29 |
| Cement CEM I 42.5N | CEMENT-42.5 | kg | 2523.29 |
| Quarry dust | QUARRY-DUST | kg | 2517.49 |
| Ballast 6 mm (1/4 inch chips) | BALLAST-6MM | kg | 2517.10 |
| Red iron oxide pigment | PIGMENT-RED-OXIDE | kg | 2821.10 |
| Raw water (borehole or mains) | WATER-RAW | L |
Units besides kg: bag50 = 50 kg bag (50 kg) , pallet60 = Pallet of 60 blocks (60 pcs) , pallet10m2 = Pallet of 10 m² pavers (10 m2)
What the factory makes
Block dry mix (mix ratio by % weight)
| In | Code | Share |
|---|---|---|
| Cement CEM II 32.5N | CEMENT-32.5 | 11 % |
| Quarry dust | QUARRY-DUST | 59 % |
| Ballast 6 mm (1/4 inch chips) | BALLAST-6MM | 30 % |
| Out | Code | Kind | Yield |
|---|---|---|---|
| Block dry mix (1 : 5.4 : 2.7) | DRY-MIX-BLOCK | Main product | 97–100 % |
| Waste | WASTE | Waste | 0–3 % |
Steps: Batching by weight → Dry mixing
Paver dry mix, red (mix ratio by % weight)
| In | Code | Share |
|---|---|---|
| Cement CEM I 42.5N | CEMENT-42.5 | 18 % |
| Quarry dust | QUARRY-DUST | 50 % |
| Ballast 6 mm (1/4 inch chips) | BALLAST-6MM | 31.5 % |
| Red iron oxide pigment | PIGMENT-RED-OXIDE | 0.5 % |
| Out | Code | Kind | Yield |
|---|---|---|---|
| Paver dry mix, red | DRY-MIX-PAVER | Main product | 97–100 % |
| Waste | WASTE | Waste | 0–3 % |
Steps: Batching by weight → Dry mixing with pigment
Hollow block 6 in (about 17 kg fresh)
| In | Code | Share |
|---|---|---|
| Block dry mix (1 : 5.4 : 2.7) | DRY-MIX-BLOCK | |
| Raw water (borehole or mains) | WATER-RAW |
| Out | Code | Kind | Yield |
|---|---|---|---|
| Hollow concrete block 6 in (150 × 200 × 400 mm) | BLOCK-6IN | Main product | |
| Waste | WASTE | Waste |
Steps: Wet mixing, pressing and vibrating (4 blocks per cycle) → Move to the curing yard, water daily
Zigzag paver 80 mm red, per m² (about 180 kg)
| In | Code | Share |
|---|---|---|
| Paver dry mix, red | DRY-MIX-PAVER | |
| Raw water (borehole or mains) | WATER-RAW |
| Out | Code | Kind | Yield |
|---|---|---|---|
| Zigzag paver 80 mm, red | PAVER-ZZ80-RED | Main product | |
| Waste | WASTE | Waste |
Steps: Wet mixing, pressing and vibrating → Move to the curing yard, cover and water daily
Yield is the share of the input weight, as a range seen in practice. The factory records the real weights on every run.
All products and intermediates
| Item | Code | Unit | HS code |
|---|---|---|---|
| Block dry mix (1 : 5.4 : 2.7) | DRY-MIX-BLOCK | kg | |
| Paver dry mix, red | DRY-MIX-PAVER | kg | |
| Hollow concrete block 6 in (150 × 200 × 400 mm) | BLOCK-6IN | pcs | 6810.11 |
| Zigzag paver 80 mm, red | PAVER-ZZ80-RED | m2 | 6810.19 |
Quality checks
Aggregate and cement intake intake
Every lorry of aggregate; cement per delivery
| Parameter | Accepted | |
|---|---|---|
| Silt and clay content (aggregates) | ≤ 8 % | critical: a failure holds the lot |
| Grading and cleanliness (no soil, organic matter) | pass / fail | critical: a failure holds the lot |
| Cement bags: KEBS mark, not older than 3 months, not lumpy | pass / fail | critical: a failure holds the lot |
| Weighbridge net weight against the delivery note | measured |
Block release after curing release
Crush 3 blocks per production day at 7 and 28 days; lot stays in the curing yard until released
| Parameter | Accepted | |
|---|---|---|
| Days cured before release | ≥ 7 days | critical: a failure holds the lot |
| Compressive strength at 7 days (gross area) | ≥ 2.5 N/mm2 | critical: a failure holds the lot |
| Compressive strength at 28 days (gross area) | ≥ 3.5 N/mm2 | |
| Dimensions within ±3 mm, square edges, no cracks | pass / fail | critical: a failure holds the lot |
| Water absorption | ≤ 12 % |
Paver release after curing release
Test 4 pavers per production day at 14 and 28 days; lot stays in the curing yard until released
| Parameter | Accepted | |
|---|---|---|
| Days cured before release | ≥ 14 days | critical: a failure holds the lot |
| Compressive strength (corrected) | ≥ 40 N/mm2 | critical: a failure holds the lot |
| Water absorption | ≤ 6 % | |
| Thickness 80 mm ±3 mm, colour even | pass / fail | critical: a failure holds the lot |
Results travel in run.completed (quality) and a hold in lot.hold_changed.
Example messages
1. You send a consignment
POST /api/v1/consignments. Here as toll work (the sender keeps ownership and pays for processing); leave out mode to sell the goods to the factory.
{
"reference_no": "VAB-26-7",
"source": "society_api",
"kind": "value_addition",
"mode": "toll",
"sender": {
"external_system": "your-system",
"society_id": 39,
"name": "Example Supplier Ltd"
},
"item": {
"code": "QUARRY-DUST"
},
"declared_qty": 1000,
"unit": "kg",
"dispatched_at": "2026-11-15T08:10:00+03:00",
"lots": [
{
"lot_no": "LOT-001",
"qty": 1000
}
]
}
2. You receive the results
Webhook run.completed, for 1,000 kg in (the middle of each yield range). Main products and co-products carry their grade when the item is one of a graded family; quality carries the checks recorded on the run.
{
"type": "run.completed",
"data": {
"reference_no": "VAB-26-7",
"work_order_ref": "WO-26-0042",
"item": "DRY-MIX-BLOCK",
"completed_at": "2026-11-16T17:30:00+03:00",
"outturn_no": "LOT-…",
"yield_pct": 98.5,
"outputs": [
{
"item": "DRY-MIX-BLOCK",
"grade": "BLOCK",
"role": "main",
"qty": 985,
"unit": "kg",
"lot_no": "LOT-…",
"yield_flag": null,
"bags": null,
"bag_unit": null,
"packets": null
},
{
"item": "WASTE",
"grade": null,
"role": "waste",
"qty": 15,
"unit": "kg",
"lot_no": "LOT-…",
"yield_flag": null,
"bags": null,
"bag_unit": null,
"packets": null
}
],
"quality": []
}
}